Residual stress and damage-induced critical fracture on CO2laser treated fused silica (English)
- New search for: Matthews, M. J.
- New search for: Stolken, J. S.
- New search for: Vignes, R. M.
- New search for: Norton, M. A.
- New search for: Yang, S.
- New search for: Cooke, J. D.
- New search for: Guss, G. M.
- New search for: Adams, J. J.
- New search for: Matthews, M. J.
- New search for: Stolken, J. S.
- New search for: Vignes, R. M.
- New search for: Norton, M. A.
- New search for: Yang, S.
- New search for: Cooke, J. D.
- New search for: Guss, G. M.
- New search for: Adams, J. J.
In:
Proc. SPIE
;
7504
; 750410
;
2009
-
ISBN:
-
ISSN:
- Conference paper / Electronic Resource
-
Title:Residual stress and damage-induced critical fracture on CO2laser treated fused silica
-
Contributors:Matthews, M. J. ( author ) / Stolken, J. S. ( author ) / Vignes, R. M. ( author ) / Norton, M. A. ( author ) / Yang, S. ( author ) / Cooke, J. D. ( author ) / Guss, G. M. ( author ) / Adams, J. J. ( author )
-
Conference:Laser-Induced Damage in Optical Materials: 2009 ; 2009 ; Boulder,Colorado,United States
-
Published in:Proc. SPIE ; 7504 ; 750410
-
Publisher:
- New search for: SPIE
-
Publication date:2009-12-29
-
ISBN:
-
ISSN:
-
DOI:
-
Type of media:Conference paper
-
Type of material:Electronic Resource
-
Language:English
-
Source:
Table of contents conference proceedings
The tables of contents are generated automatically and are based on the data records of the individual contributions available in the index of the TIB portal. The display of the Tables of Contents may therefore be incomplete.
- 75040A
-
Design consideration for high damage threshold UV-Vis-IR mirrorsPervak, V. / Trubetskov, M. / Tikhonravov, A. et al. | 2009
- 75040B
-
Investigation in oxide mixture coatings with adapted gradient index profilesStarke, Kai / Jensen, Lars O. / Jupé, Marco / Ristau, Detlev / Abromavicius, Giedrius / Juskevicius, Kestutis / Buzelis, Rytis / Drazdys, Ramutis et al. | 2009
- 75040C
-
Meeting thin film design and production challenges for laser damage resistant optical coatings at the Sandia Large Optics Coating OperationBellum, John / Kletecka, Damon / Rambo, Patrick / Smith, Ian / Kimmel, Mark / Schwarz, Jens / Geissel, Matthias / Copeland, Guild / Atherton, Briggs / Smith, Douglas et al. | 2009
- 75040D
-
Influence of subsurface defects on 355 nm laser damage resistance of monolayer and multilayer coatingsHu, Guohang / Shao, Shuying / Yang, Minghong / Shao, Jianda / Zhao, Yuanan / Yi, Kui / Fan, Zhengxiu et al. | 2009
- 75040E
-
Anti-reflection coating damage threshold dependence on substrate materialLyngnes, Ove / Ode, Aiko / Ness, Dale C. et al. | 2009
- 75040F
-
Optical coatings with ultralow refractive index SiO2filmsWang, Jue / Zhou, Bin / Shen, Jun / Wu, Guangming et al. | 2009
- 75040G
-
Ultrafast laser-induced modifications of energy bands of non-metal crystalsGruzdev, Vitaly et al. | 2009
- 75040H
-
Laser-induced damage and nonlinear absorption of ultrashort laser pulses in the bulk of fused silicaTurowski, M. / Jupé, M. / Jensen, L. / Ristau, D. et al. | 2009
- 75040I
-
Influence of Na-related defects on DUV nonlinear absorption in CaF2: nanosecond versus femtosecond laser pulsesMühlig, Ch. / Stafast, H. / Triebel, W. / Zeuner, Th. / Karras, Ch. / Letz, M. et al. | 2009
- 75040J
-
A microscopic model for long-term laser damage in calcium fluorideRix, Stephan / Natura, Ute / Letz, Martin / Felser, Claudia / Parthier, Lutz et al. | 2009
- 75040K
-
Biaxial flexural strength of optical window materialsKlein, Claude A. et al. | 2009
- 75040L
-
Modeling wet chemical etching of surface flaws on fused silicaFeit, M. D. / Suratwala, T. I. / Wong, L. L. / Steele, W. A. / Miller, P. E. / Bude, J. D. et al. | 2009
- 75040M
-
Modeling of light intensification by conical pits within multilayer high reflector coatingsQiu, S. Roger / Wolfe, Justin E. / Monterrosa, Anthony M. / Feit, Michael D. / Pistor, Thomas V. / Stolz, Christopher J. et al. | 2009
- 75040N
-
Analysis in wavelength dependence of electronic damageJupé, M. / Jensen, L. / Starke, K. / Ristau, D. / Melninkaitis, A. / Sirutkaitis, V. et al. | 2009
- 75040O
-
Time-resolved digital holography: a versatile tool for femtosecond laser-induced damage studiesMelninkaitis, Andrius / Balciunas, Tadas / Vanagas, Andrius / Sirutkaitis, Valdas et al. | 2009
- 75040P
-
Fundamental processes controlling the single and multiple femtosecond pulse damage behavior of dielectric oxide filmsEmmert, L. A. / Nguyen, D. N. / Mero, M. / Rudolph, W. / Ristau, D. / Starke, K. / Jupé, M. / Menoni, C. S. / Patel, D. / Krous, E. et al. | 2009
- 75040Q
-
Subpicosecond pulse laser damage behavior of dielectric thin films prepared by different techniquesMangote, B. / Gallais, L. / Commandré, M. / Zerrad, M. / Natoli, J. Y. / Lequime, M. et al. | 2009
- 75040R
-
Mixed metal dielectric gratings for pulse compression applicationsNéauport, J. / Palmier, S. / Bonod, N. / Lavastre, E. / Baclet, N. / Dupuy, G. et al. | 2009
- 75040S
-
Thin film femtosecond laser damage competitionStolz, Christopher J. / Ristau, Detlev / Turowski, Marcus / Blaschke, Holger et al. | 2009
- 75040T
-
Aspects of laser optics qualification for space applicationsRiede, Wolfgang / Allenspacher, Paul / Schröder, Helmut / Mahnke, Peter / Paunescu, Gabriela / Wernham, Denny et al. | 2009
- 75040U
-
The effects on glass surfaces of shrapnel and debris emissions from Petawatt laser driven solid targetsAndrew, James E. / Wallace, Katherine A. et al. | 2009
- 75040V
-
Impact of outgassing organic contamination on laser induced damage of opticsBien-Aimé, K. / Pereira, A. / Belin, C. / Gallais, L. / Grua, P. / Tovena-Pecault, I. / Néauport, J. / Fargin, E. et al. | 2009
- 75040W
-
Chemical characterizations of optical materials: a tool for high quality componentsAmbard, C. / Rondeau, O. / Destribats, J. / Cormont, P. / Néauport, J. et al. | 2009
- 75040X
-
Laser damage precursors in fused silicaMiller, P. E. / Suratwala, T. I. / Bude, J. D. / Laurence, T. A. / Shen, N. / Steele, W. A. / Feit, M. D. / Menapace, J. A. / Wong, L. L. et al. | 2009
- 75040Y
-
Diagnostics tools for subsurface damage characterization of ground silica partsCormont, P. / Neauport, J. / Darbois, N. / Destribats, J. / Ambard, C. / Rondeau, O. et al. | 2009
- 75040Z
-
Birefringence and residual stress induced by CO2 laser mitigation of damage growth in fused silicaGallais, L. / Cormont, P. / Rullier, J. L. et al. | 2009
- 75041A
-
Early thermal damage in optical coatings identified by infrared spectral signaturesKim, Sangho S. / Gabriel, Nicholas T. / Chan, Wing S. / Talghader, Joseph J. et al. | 2009
- 75041B
-
Process for rapid detection of fratricidal defects on optics using linescan phase-differential imagingRavizza, Frank L. / Nostrand, Michael C. / Kegelmeyer, Laura M. / Hawley, Ruth A. / Johnson, Michael A. et al. | 2009
- 75041C
-
Laser-induced surface damage density measurements of fused silica optics: a parametric studyLamaignère, Laurent / Reyné, Stéphane / Donval, Thierry / Courchinoux, Roger / Poncetta, Jean-Christophe / Bertussi, Bertrand / Bercegol, H. et al. | 2009
- 75041D
-
Numerical analysis of laser-induced damage threshold search algorithms and their uncertaintyMelninkaitis, Andrius / Bataviciute, Gintaré / Sirutkaitis, Valdas et al. | 2009
- 75041E
-
Spot-size dependence of the LIDT from the NIR to the UVJensen, L. / Schrameyer, S. / Jupé, M. / Blaschke, H. / Ristau, D. et al. | 2009
- 75041F
-
Adaptive laser-induced damage detectionMelninkaitis, Andrius / Mirauskas, Julius / Sirutkaitis, Valdas et al. | 2009
- 75041G
-
Optical damage testing at the Z-Backlighter facility at Sandia National LaboratoriesKimmel, Mark / Rambo, Patrick / Broyles, Robin / Geissel, Matthias / Schwarz, Jens / Bellum, John / Atherton, Briggs et al. | 2009
- 75041H
-
Angle resolved scattering: a method for in situ investigations of laser-induced damage?Schröder, Sven / Herffurth, Tobias / Duparré, Angela et al. | 2009
- 75041I
-
Life testing for laser optics: a first lookArenberg, Jonathan W. et al. | 2009
- 75041J
-
Damage and degradation of optics and sensors under intense EUV radiation from a table-top laser produced plasma sourceBarkusky, Frank / Bayer, Armin / Flöter, Bernhard / Peth, Christian / Mann, Klaus et al. | 2009
- 75041K
-
Modeling laser conditioning of KDP crystalsDuchateau, Guillaume et al. | 2009
- 75041L
-
Laser conditioning process combining N/1 and S/1 programs to improve the damage resistance of KDP crystalsZhao, Yuanan / Hu, Guohang / Shao, Jianda / Liu, Xiaofeng / He, Hongbo / Fan, Zhengxiu et al. | 2009
- 75041M
-
Nanosecond-laser induced damage at 1064 nm, 532 nm, and 355 nm in LiB3O5Wagner, Frank R. / Hildenbrand, Anne / Natoli, Jean-Yves / Commandre, Mireille et al. | 2009
- 75041N
-
Laser induced damage of sapphire and titanium doped sapphire crystals under femtosecond to nanosecond laser irradiationBussière, B. / Utéza, O. / Sanner, N. / Sentis, M. / Riboulet, G. / Vigroux, L. / Commandré, M. / Wagner, F. / Natoli, J.-Y. / Chambaret, J.-P. et al. | 2009
- 75041O
-
Deterministic single shot and multiple shots bulk damage thresholds for doped and undoped crystalline and ceramic YAGDo, Binh T. / Smith, Arlee V. et al. | 2009
- 75041P
-
Study of haze in 193nm high dose irradiated CaF2crystalsNatura, Ute / Rix, Stephan / Letz, Martin / Parthier, Lutz et al. | 2009
- 75041Q
-
Development of large size MgF2single crystal grown by the CZ methodAriyuki, Masao / Hashimoto, Yasuhiro / Mochizuki, Naoto / Inui, Yoji / Masada, Isao / Nawata, Teruhiko / Fukuda, Tsuguo et al. | 2009
- 75041R
-
Laser-induced damage thresholds in silica glasses at different temperatureMikami, K. / Motokoshi, S. / Fujita, M. / Jitsuno, T. / Kawanaka, J. / Yasuhara, R. et al. | 2009
- 750401
-
Front Matter: Volume 7504| 2009
- 750402
-
The effect of nitrogen doping on the multiple-pulse subpicosecond dielectric breakdown of hafnia filmsNguyen, D. N. / Emmert, L. A. / Rudolph, W. / Patel, D. / Krous, E. / Menoni, C. S. et al. | 2009
- 750403
-
Studies of femtosecond laser induced damage of HfO2thin film in atmospheric and vacuum environmentsNguyen, D. N. / Emmert, L. A. / Rudolph, W. / Patel, D. / Krous, E. / Menoni, C. S. / Shinn, M. et al. | 2009
- 750404
-
Surface damage of thin AlN films with increased oxygen content by nanosecond and femtosecond laser pulsesGruzdev, Vitaly / Salakhutdinov, Ildar / Chen, J. K. / Danylyuk, Yuriy / McCullen, Erik / Auner, Gregory et al. | 2009
- 750405
-
Laser damage resistant pits in dielectric coatings created by femtosecond laser machiningWolfe, Justin / Qiu, Roger / Stolz, Christopher / Thomas, Michael / Martinez, Carolyn / Ozkan, Arzu et al. | 2009
- 750406
-
Thermal robustness of ion beam sputtered TiO2/SiO2, TiO2/Al2O3and Al2O3/SiO2IR anti-reflective coatings on YAG and sapphire substratesNess, Dale C. / Traggis, Nick / Lyngnes, Ove et al. | 2009
- 750407
-
Optimization of scandia thin films for high power laser coating applicationsKrous, Erik M. / Patel, Dinesh / Markosyan, Ashot / Nguyen, Duy N. / Emmert, Luke A. / Langston, Peter / Route, Roger / Fejer, Martin / Rudolph, Wolfgang / Shinn, Michelle et al. | 2009
- 750408
-
Laser conditioning of high reflectivity mirrors used in OPOs by 266 and 355 nm nanosecond pulsesMelninkaitis, Andrius / Vaninas, Arturas / Mirauskas, Julius / Kuršelis, Kestutis / Balachninaite, Ona / Sirutkaitis, Valdas et al. | 2009
- 750409
-
193 nm laser induced spectral shift in HR coated mirrorsCho, Byungil / Rudisill, J. Earl / Danielewicz, Edward et al. | 2009
- 750410
-
Residual stress and damage-induced critical fracture on CO2laser treated fused silicaMatthews, M. J. / Stolken, J. S. / Vignes, R. M. / Norton, M. A. / Yang, S. / Cooke, J. D. / Guss, G. M. / Adams, J. J. et al. | 2009
- 750411
-
Study of CO2laser smoothing of surface roughness in fused silicaShen, Nan / Matthews, Manyalibo J. / Fair, James E. / Britten, Jerald A. / Nguyen, Hoang T. / Cooke, Juliet D. / Elhadj, Selim / Henshaw, William D. / Guss, Gabe M. / Bass, Isaac L. et al. | 2009
- 750412
-
The effect of pulse duration on the growth rate of laser-induced damage sites at 351 nm on fused silica surfacesNegres, R. A. / Norton, M. A. / Liao, Z. M. / Cross, D. A. / Bude, J. D. / Carr, C. W. et al. | 2009
- 750414
-
Magnetorheological finishing (MRF) of potassium dihydrogen phosphate (KDP) crystals: nonaqueous fluids development, optical finish, and laser damage performance at 1064 nm and 532 nmMenapace, J. A. / Ehrmann, P. R. / Bickel, R. C. et al. | 2009
- 750415
-
Nonlinear spectroscopy: absorption and refractionVan Stryland, Eric / Hagan, David / Webster, Scott / Padilha, Lazaro et al. | 2009
- 750416
-
Ultrafast photoluminescence as a diagnostic for laser damage initiationLaurence, Ted A. / Bude, Jeff D. / Shen, Nan / Miller, Phillip E. / Steele, William A. / Guss, Gabe / Adams, John J. / Wong, Lana L. / Feit, Michael D. / Suratwala, Tayyab I. et al. | 2009
- 750417
-
Photoluminescence and photothermal deflection measurements in KDP crystals for high power applicationsCiapponi, Alessandra / Wagner, Frank / Natoli, Jean-Yves / Bertussi, Bertrand / Guillet, François et al. | 2009
- 750418
-
Imaging system to measure kinetics of material cluster ejection during exit-surface damage initiation and growth in fused silicaRaman, Rajesh N. / Negres, Raluca A. / Demos, Stavros G. et al. | 2009
- 750419
-
High temperature thermographic measurements of laser heated silicaElhadj, Selim / Yang, Steven T. / Matthews, Manyalibo J. / Cooke, Diane J. / Bude, Jeffrey D. / Johnson, Michael / Feit, Michael / Draggoo, Vaughn / Bisson, Scott E. et al. | 2009
-
Meeting thin film design and production challenges for laser damage resistant optical coatings at the Sandia Large Optics Coating Operation [7504-20]Bellum, J. / Kletecka, D. / Rambo, P. / Smith, I. / Kimmel, M. / Schwarz, J. / Geissel, M. / Copeland, G. / Atherton, B. / Smith, D. et al. | 2009
-
Design consideration for high damage threshold UV-Vis-IR mirrors [7504-02]Pervak, V. / Trubetskov, M. / Tikhonravov, A. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Chemical characterizations of optical materials: a tool for high quality components [7504-58]Ambard, C. / Rondeau, O. / Destribats, J. / Cormont, P. / Neauport, J. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Photoluminescence and photothermal deflection measurements in KDP crystals for high power applications [7504-66]Ciapponi, A. / Wagner, F. / Natoli, J.-Y. / Bertussi, B. / Guillet, F. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Damage and degradation of optics and sensors under intense EUV radiation from a table-top laser produced plasma source [7504-73]Barkusky, F. / Bayer, A. / Floter, B. / Peth, C. / Mann, K. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Ultrafast laser-induced modifications of energy bands of non-metal crystals (Invited Paper) [7504-27]Gruzdev, V. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Analysis in wavelength dependence of electronic damage [7504-30]Jupe, M. / Jensen, L. / Starke, K. / Ristau, D. / Melninkaitis, A. / Sirutkaitis, V. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Modeling of light intensification by conical pits within multilayer high reflector coatings [7504-28]Qiu, S.R. / Wolfe, J.E. / Monterrosa, A.M. / Feit, M.D. / Pistor, T.V. / Stolz, C.J. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Time-resolved digital holography: a versatile tool for femtosecond laser-induced damage studies [7504-31]Melninkaitis, A. / Balciunas, T. / Vanagas, A. / Sirutkaitis, V. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Thin film femtosecond laser damage competition [7504-54]Stolz, C.J. / Ristau, D. / Turowski, M. / Blaschke, H. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Angle resolved scattering: a method for in situ investigations of laser-induced damage? [7504-82]Schroder, S. / Herffurth, T. / Duparre, A. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Nanosecond-laser induced damage at 1064 nm, 532 nm, and 355 nm in LiB~3O~5 [7504-76]Wagner, F.R. / Hildenbrand, A. / Natoli, J.-Y. / Commandre, M. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Surface damage of thin AlN films with increased oxygen content by nanosecond and femtosecond laser pulses [7504-11]Gruzdev, V. / Salakhutdinov, I. / Chen, J.K. / Danylyuk, Y. / McCullen, E. / Auner, G. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Fundamental processes controlling the single and multiple femtosecond pulse damage behavior of dielectric oxide films [7504-32]Emmert, L.A. / Nguyen, D.N. / Mero, M. / Rudolph, W. / Ristau, D. / Starke, K. / Jupe, M. / Menoni, C.S. / Patel, D. / Krous, E. et al. | 2009
-
Nonlinear spectroscopy: absorption and refraction (Best Oral Paper Award, Invited Paper) [7504-64]Van Stryland, E. / Hagan, D. / Webster, S. / Padilha, L. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Thermal robustness of ion beam sputtered TiO~2/SiO~2, TiO~2/Al~2O~3, and Al~2O~3/SiO~2 IR anti-reflective coatings on YAG and sapphire substrates [7504-13]Ness, D.C. / Traggis, N. / Lyngnes, O. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Aspects of laser optics qualification for space applications (Invited Paper) [7504-55]Riede, W. / Allenspacher, P. / Schroder, H. / Mahnke, P. / Paunescu, G. / Wernham, D. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Diagnostics tools for subsurface damage characterization of ground silica parts [7504-36]Cormont, P. / Neauport, J. / Darbois, N. / Destribats, J. / Ambard, C. / Rondeau, O. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Laser-induced surface damage density measurements of fused silica optics: a parametric study [7504-71]Lamaignere, L. / Reyne, S. / Donval, T. / Courchinoux, R. / Poncetta, J.-C. / Bertussi, B. / Bercegol, H. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Process for rapid detection of fratricidal defects on optics using linescan phase-differential imaging [7504-70]Ravizza, F.L. / Nostrand, M.C. / Kegelmeyer, L.M. / Hawley, R.A. / Johnson, M.A. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Laser induced damage of sapphire and titanium doped sapphire crystals under femtosecond to nanosecond laser irradiation [7504-77]Bussiere, B. / Uteza, O. / Sanner, N. / Sentis, M. / Riboulet, G. / Vigroux, L. / Commandre, M. / Wagner, F. / Natoli, J.-Y. / Chambaret, J.-P. et al. | 2009
-
Study of haze in 193nm high dose irradiated CaF~2 crystals [7504-50]Natura, U. / Rix, S. / Letz, M. / Parthier, L. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Development of large size MgF~2 single crystal grown by the CZ method [7504-52]Ariyuki, M. / Hashimoto, Y. / Mochizuki, N. / Inui, Y. / Masada, I. / Nawata, T. / Fukuda, T. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Optical coatings with ultralow refractive index SiO~2 films [7504-23]Wang, J. / Zhou, B. / Shen, J. / Wu, G. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
A microscopic model for long-term laser damage in calcium fluoride [7504-04]Rix, S. / Natura, U. / Letz, M. / Felser, C. / Parthier, L. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Residual stress and damage-induced critical fracture on CO~2 laser treated fused silica [7504-60]Matthews, M.J. / Stolken, J.S. / Vignes, R.M. / Norton, M.A. / Yang, S. / Cooke, J.D. / Guss, G.M. / Adams, J.J. / SPIE (Society) / United States et al. | 2009
-
High temperature thermographic measurements of laser heated silica [7504-68]Elhadj, S. / Yang, S.T. / Matthews, M.J. / Cooke, D.J. / Bude, J.D. / Johnson, M. / Feit, M. / Draggoo, V. / Bisson, S.E. / SPIE (Society) et al. | 2009
-
Life testing for laser optics: a first look [7504-72]Arenberg, J.W. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Deterministic single shot and multiple shots bulk damage thresholds for doped and undoped crystalline and ceramic YAG [7504-78]Do, B.T. / Smith, A.V. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Laser-induced damage thresholds in silica glasses at different temperatures [7504-47]Mikami, K. / Motokoshi, S. / Fujita, M. / Jitsuno, T. / Kawanaka, J. / Yasuhara, R. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
The effect of nitrogen doping on the multiple-pulse subpicosecond dielectric breakdown of hafnia films [7504-10]Nguyen, D.N. / Emmert, L.A. / Rudolph, W. / Patel, D. / Krous, E. / Menoni, C.S. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Investigation in oxide mixture coatings with adapted gradient index profiles [7504-19]Starke, K. / Jensen, L.O. / Jupe, M. / Ristau, D. / Abromavicius, G. / Juskevicius, K. / Buzelis, R. / Drazdys, R. / SPIE (Society) / United States et al. | 2009
-
The effects on glass surfaces of shrapnel and debris emissions from Petawatt laser driven solid targets [7504-56]Andrew, J.E. / Wallace, K.A. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Laser-induced damage and nonlinear absorption of ultrashort laser pulses in the bulk of fused silica [7504-05]Turowski, M. / Jupe, M. / Jensen, L. / Ristau, D. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Impact of outgassing organic contamination on laser-induced damage of optics [7504-57]Bien-Aime, K. / Pereira, A. / Belin, C. / Gallais, L. / Grua, P. / Tovena-Pecault, I. / Neauport, J. / Fargin, E. / SPIE (Society) / United States et al. | 2009
-
Birefringence and residual stress induced by CO~2 laser mitigation of damage growth in fused silica [7504-37]Gallais, L. / Cormont, P. / Rullier, J.L. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Early thermal damage in optical coatings identified by infrared spectral signatures [7504-69]Kim, S.S. / Gabriel, N.T. / Chan, W.S. / Talghader, J.J. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Optical damage testing at the Z-Backlighter facility at Sandia National Laboratories [7504-45]Kimmel, M. / Rambo, P. / Broyles, R. / Geissel, M. / Schwarz, J. / Bellum, J. / Atherton, B. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Optimization of scandia thin films for high power laser coating applications [7504-15]Krous, E.M. / Patel, D. / Markosyan, A. / Nguyen, D.N. / Emmert, L.A. / Langston, P. / Route, R. / Fejer, M. / Rudolph, W. / Shinn, M. et al. | 2009
-
193 nm laser induced spectral shift in HR coated mirrors [7504-17]Cho, B. / Rudisill, J.E. / Danielewicz, E. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Anti-reflection coating damage threshold dependence on substrate material [7504-22]Lyngnes, O. / Ode, A. / Ness, D.C. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Biaxial flexural strength of optical window materials [7504-26]Klein, C.A. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Modeling wet chemical etching of surface flaws on fused silica [7504-29]Feit, M.D. / Suratwala, T.I. / Wong, L.L. / Steele, W.A. / Miller, P.E. / Bude, J.D. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Influence of Na-related defects on DUV nonlinear absorption in CaF~2: nanosecond versus femtosecond laser pulses (Best Poster Paper Award) [7504-03]Muhlig, C. / Stafast, H. / Triebel, W. / Zeuner, T. / Karras, C. / Letz, M. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Numerical analysis of laser-induced damage threshold search algorithms and their uncertainty [7504-42]Melninkaitis, A. / Bataviciute, G. / Sirutkaitis, V. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Laser conditioning of high reflectivity mirrors used in OPOs by 266 and 355 nm nanosecond pulses [7504-16]Melninkaitis, A. / Vaninas, A. / Mirauskas, J. / Kurselis, K. / Balachninaite, O. / Sirutkaitis, V. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Subpicosecond pulse laser damage behavior of dielectric thin films prepared by different techniques [7504-33]Mangote, B. / Gallais, L. / Commandre, M. / Zerrad, M. / Natoli, J.Y. / Lequime, M. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Laser damage precursors in fused silica [7504-59]Miller, P.E. / Suratwala, T.I. / Bude, J.D. / Laurence, T.A. / Shen, N. / Steele, W.A. / Feit, M.D. / Menapace, J.A. / Wong, L.L. / SPIE (Society) et al. | 2009
-
The effect of pulse duration on the growth rate of laser-induced damage sites at 351 nm on fused silica surfaces [7504-61]Negres, R.A. / Norton, M.A. / Liao, Z.M. / Cross, D.A. / Bude, J.D. / Carr, C.W. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Adaptive laser-induced damage detection [7504-44]Melninkaitis, A. / Mirauskas, J. / Sirutkaitis, V. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Laser conditioning process combining N/1 and S/1 programs to improve the damage resistance of KDP crystals [7504-75]Zhao, Y. / Hu, G. / Shao, J. / Liu, X. / He, H. / Fan, Z. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Influence of subsurface defects on 355 nm laser damage resistance of monolayer and multilayer coatings [7504-21]Hu, G. / Shao, S. / Yang, M. / Shao, J. / Zhao, Y. / Yi, K. / Fan, Z. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Mixed metal dielectric gratings for pulse compression applications [7504-53]Neauport, J. / Palmier, S. / Bonod, N. / Lavastre, E. / Baclet, N. / Dupuy, G. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Studies of femtosecond laser-induced damage of HfO~2 thin film in atmospheric and vacuum environments [7504-09]Nguyen, D.N. / Emmert, L.A. / Rudolph, W. / Patel, D. / Krous, E. / Menoni, C.S. / Shinn, M. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Laser damage resistant pits in dielectric coatings created by femtosecond laser machining [7504-12]Wolfe, J. / Qiu, R. / Stolz, C. / Thomas, M. / Martinez, C. / Ozkan, A. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Study of CO~2 laser smoothing of surface roughness in fused silica [7504-62]Shen, N. / Matthews, M.J. / Fair, J.E. / Britten, J.A. / Nguyen, H.T. / Cooke, J.D. / Elhadj, S. / Henshaw, W.D. / Guss, G.M. / Bass, I.L. et al. | 2009
-
Magnetorheological finishing (MRF) of potassium dihydrogen phosphate (KDP) crystals: nonaqueous fluids development, optical finish, and laser damage performance at 1064 nm and 532 nm [7504-63]Menapace, J.A. / Ehrmann, P.R. / Bickel, R.C. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Ultrafast photoluminescence as a diagnostic for laser damage initiation [7504-65]Laurence, T.A. / Bude, J.D. / Shen, N. / Miller, P.E. / Steele, W.A. / Guss, G. / Adams, J.J. / Wong, L.L. / Feit, M.D. / Suratwala, T.I. et al. | 2009
-
Imaging system to measure kinetics of material cluster ejection during exit-surface damage initiation and growth in fused silica [7504-67]Raman, R.N. / Negres, R.A. / Demos, S.G. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Spot-size dependence of the LIDT from the NIR to the UV [7504-43]Jensen, L. / Schrameyer, S. / Jupe, M. / Blaschke, H. / Ristau, D. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009
-
Modeling laser conditioning of KDP crystals [7504-74]Duchateau, G. / SPIE (Society) / United States / Pacific Northwest National Laboratory (U.S.) et al. | 2009